High-grade heavy metal elements in copper slag (CS) are worth recovering. Unfortunately, the high viscosity of leaching solution, low leaching efficiency, difficult filtration and low separation efficiency of valuable components exist in the traditional sulfuric acid leaching process. In this study, the above problems are solved by sulfuric acid pretreatment + curing + water leaching. Moreover, iron, cobalt and copper ions in solution are separated by stepwise precipitation. The final iron, cobalt, copper and silicon recoveries are 99.01 %, 98.45 %, 93.13 % and 99.52 %, respectively. Thermodynamic calculations show that H